1) The wood layers are heated at certain temperatures to reduce the moisture to the appropriate rates according to blades' characteristics.

 

 

2)With the caliber machine we developed , the wood layer thicknesses are equalized with 10 %precision of a millimeter.

 

 

3)The wood layers are cut in the blade form with the cnc machine ,we do not cut the blade after the manufacturing

4)The middle layers are covered with the required amount of adhesive with the glue application apparatus we developed ; than pressed  with vacuum press system .

5) After 24 hours of desiccation process the top of the middle layers is covered with carbon  and epoxy ;

than with vacuum press system it is pressed with the top surface wood  layers and finally it is heated in appropriate heat .   .

 

 

6) After 24 hours desiccation process the edges of the blades are insulated to provide the moisture -proof quality .

 

 

7) The writings indicating the properties of the blade are written on the CNC writing machine .

 

 

8) Blade's edges are insulated to ensure moisture - proof feature.

 

9) The blade is covered with varnish. The second layer varnish applied on the blade has a rough structure to better hold the water-based rubber adhesive .

 

10) The handle wood layers are combined with the press method , than they are shaped by milling .

 

11) The head and handle are combined with two dowels to finish the production .

 

 

12) Finally , with the milling machine a space is opened on the handle and a round wooden badge with A&O logo is mounted.